DISPERSING AND LEVELING AGENTS


Concentrate dispersion and egalize material
PRODUCTION SPECIFICATION

Chemical Composition : Combination of suitable non-ionic ether and esters
Ionic Character : Non-ionic
Appearence : Light yellow clear,voscous liquid
Ph : 6-7

PROPERTIES : *ALT EGA X 100 is a perfec disperse and egalize material
* It is foam regulated.
* It is supply uniform leveling dispers dye in poliester dyeing İndantren and reactive dye in cottons dyeing ,kationic dye goups in acrilic dyeing, acid,crom and metal complex dyes inwool dyeing baths.
* It is prevent aglomeration and waste on dying equipment
* It is proved perfect smooh dyeing handle.
* It is prevent formation of oligomer.
* Its high stability dispers and egalize metaril so,it is perfect work in high temperature and high pressure for dyeing poliester and their mixtures.
* There is needlessness washing process after dyeing because of prevent formation of oligomer.
* It is mix with water in all ratio.
* It is used with non-ionic,anionic and cationic dyes , auxiliary chemicals ,acids,salt etc.
* It is used with all kind of carrier.
* It is used for dyeing knitting ,weawing fabrics,bobbin,carpet and fibres dyeing.

APPLICATION * The bath temperature is adjuct to 50-60 C
* The ph value is regulate 4.5-5
* Add in dyeing bath 0.3-0.6 g/lt ALT EGA X 100. İf need you can a add other auxiliary chemicals in bath .
* Operate the machine 5 minutes before adding dyestuff.
* Add the dyestuff which is filtered than work the machine .10-15 min İn 50-60 C bath temperature.
* Increase the bath temperature to 130 C by the 1-1,5 C/min.
* Work the machine in this 130 C temperature between 60-90 min.according to colour of light or deep.
* Reduce the bath temperature slowly to 70-80 C after finishing dyeing and than drain the water .if need make reductive washing
• Generally there is no need final cleaning operation dyeing
with ALT EGA X 100. For the correction of the poliester goods dyeing with poliester dyes in condition of HT( high temperature )
0.3-0.6 g/lt ALT EGA X 100 at 125-135 C work wachine 1 hour.and then apply below washing process.
0.3-0.6 g/lt ALT EGA X 100
1.0-2.0 g/lt sodium hydrosülfite
3.0-5.0 g/lt sodium hydroxide (35 Be)
Temperature :70 C
Time : 10-15 min.
General usage is recomended below
For diepersant : 0.3-0.6 g/lt
For egalizator : 0.5-1.0 g/lt
Extraction of dye :1.0-2.0 g/lt

STORAGE LIFE : Original package and normal temperature 6 month
PACKAGING : 60 Kg plastic carboys and 120 kg plactic barrelsWarning : All above information is best of our knowledge obtained during process and research.Every user of
our products should verify the data under his own conditions.

Concentrate dispersion and egalize material
PRODUCTION SPECIFICATION

Chemical Composition : Combination of suitable non-ionic ether and esters
Ionic Character : Non-ionic
Appearence : Light yellow clear,voscous liquid
Ph : 6-7

PROPERTIES : * ALT EGA CONZ is a perfec disperse and egalize material
* It is foam regulated.
* It is supply uniform leveling dispers dye in poliester dyeing İndantren and reactive dye in cottons dyeing ,kationic dye goups in acrilic dyeing, acid,crom and metal complex dyes inwool dyeing baths.
* It is prevent aglomeration and waste on dying equipment
* It is proved perfect smooh dyeing handle.
* It is prevent formation of oligomer.
* Its high stability dispers and egalize metaril so,it is perfect work in high temperature and high pressure for dyeing poliester and their mixtures.
* There is needlessness washing process after dyeing because of prevent formation of oligomer.
* It is mix with water in all ratio.
* It is used with non-ionic,anionic and cationic dyes , auxiliary chemicals ,acids,salt etc.
* It is used with all kind of carrier.
* It is used for dyeing knitting ,weawing fabrics,bobbin,carpet and fibres dyeing.
APPLICATION * The bath temperature is adjuct to 50-60 C
* The ph value is regulate 4.5-5
* Add in dyeing bath 0.3-0.6 g/lt ALT EGA CONZ İf need you can a add other auxiliary chemicals in bath .
* Operate the machine 5 minutes before adding dyestuff.
* Add the dyestuff which is filtered than work the machine .10-15 min İn 50-60 C bath temperature.
* Increase the bath temperature to 130 C by the 1-1,5 C/min.
* Work the machine in this 130 C temperature between 60-90 min.according to colour of light or deep.
* Reduce the bath temperature slowly to 70-80 C after finishing dyeing and than drain the water .if need make reductive washing
• Generally there is no need final cleaning operation dyeing with ALT EGA CONZ. For the correction of the poliester goods dyeing with poliester dyes in condition of HT( high temperature )
0.3-0.6 g/lt ALT EGA CONZ at 125-135 C work wachine 1 hour.and then apply below washing process.
0.3-0.6 g/lt ALT EGA CONZ
1.0-2.0 g/lt sodium hydrosülfite
3.0-5.0 g/lt sodium hydroxide (35 Be)
Temperature : 70 C
Time : 10-15 min.

General usage is recomended below
For diepersant : 0.3-0.6 g/lt
For egalizator : 0.5-1.0 g/lt
Extraction of dye :1.0-2.0 g/lt

STORAGE LIFE : Original package and normal temperature 6 month
PACKAGING : 60 Kg plastic carboys and 120 kg plactic barrels Warning : All above information is best of our knowledge obtained during process and research.Every user of
our products should verify the data under his own conditions.

Concentrate dispersion and egalize material
PRODUCTION SPECIFICATION

Chemical Composition : Combination of suitable non-ionic ether and esters
Ionic Character : Non-ionic
Appearence : Light yellow clear,voscous liquid
Ph : 6-7

PROPERTIES : * ALT EGA VS is a perfec disperse and egalize material
* It is foam regulated.
* It is supply uniform leveling dispers dye in poliester dyeing İndantren and reactive dye in cottons dyeing ,kationic dye goups in acrilic dyeing, acid,crom and metal complex dyes inwool dyeing baths.
* It is prevent aglomeration and waste on dying equipment
* It is proved perfect smooh dyeing handle.
* It is prevent formation of oligomer.
* Its high stability dispers and egalize metaril so,it is perfect work in high temperature and high pressure for dyeing poliester and their mixtures.
* There is needlessness washing process after dyeing because of prevent formation of oligomer.
* It is mix with water in all ratio.
* It is used with non-ionic,anionic and cationic dyes , auxiliary chemicals ,acids,salt etc.
* It is used with all kind of carrier.
* It is used for dyeing knitting ,weawing fabrics, bobbin, carpet and fibres dyeing.

APPLICATION * The bath temperature is adjuct to 50-60 C
* The ph value is regulate 4.5-5
* Add in dyeing bath 0.5-1.0 g/lt ALT EGA VS. İf need you can a add other auxiliary chemicals in bath .
* Operate the machine 5 minutes before adding dyestuff.
* Add the dyestuff which is filtered than work the machine .10-15 min İn 50-60 C bath temperature.
* Increase the bath temperature to 130 C by the 1-1,5 C/min.
* Work the machine in this 130 C temperature between 60-90 min.according to colour of light or deep.
* Reduce the bath temperature slowly to 70-80 C after finishing dyeing and than drain the water .if need make reductive washing
• Generally there is no need final cleaning operation dyeing
with ALT EGA VS. For the correction of the poliester goods dyeing with poliester dyes in condition of HT( high temperature )
0.5-1.0 g/lt ALT EGA VS at 125-135 C work wachine 1 hour.and then apply below washing process.
0.5-1.0 g/lt ALT EGA VS
1.0-2.0 g/lt sodium hydrosülfite
3.0-5.0 g/lt sodium hydroxide (35 Be)
Temperature : 70 C
Time : 10-15 min.
General usage is recomended below
For diepersant : 0.5-1.0 g/lt
For egalizator : 1.0-2.0 g/lt
Extraction of dye : 1.5-3.0 g/lt

STORAGE LIFE : Original package and normal temperature 6 month
PACKAGING : 60 Kg plastic carboys and 120 kg plactic barrelsWarning : All above information is best of our knowledge obtained during process and research.Every user of
our products should verify the data under his own conditions.

Concentrate dispersion and egalize material
PRODUCTION SPECIFICATION
Chemical Composition : Combination of suitable non-ionic ether and esters
Ionic Character : Non-ionic
Appearence : Light yellow clear,voscous liquid
Ph : 6-7

PROPERTIES : * ALT EGA TC is a perfec disperse and egalize material
* It is foam regulated.
* It is supply uniform leveling dispers dye in poliester dyeing İndantren and reactive dye in cottons dyeing ,kationic dye goups in acrilic dyeing, acid,crom and metal complex dyes inwool dyeing baths.
* It is prevent aglomeration and waste on dying equipment
* It is proved perfect smooh dyeing handle.
* It is prevent formation of oligomer.
* Its high stability dispers and egalize metaril so,it is perfect work in high temperature and high pressure for dyeing poliester and their mixtures.
* There is needlessness washing process after dyeing because of prevent formation of oligomer.
* It is mix with water in all ratio.
* It is used with non-ionic,anionic and cationic dyes , auxiliary chemicals ,acids,salt etc.
* It is used with all kind of carrier.
* It is used for dyeing knitting ,weawing fabrics, bobbin, carpet and fibres dyeing.
APPLICATION* The bath temperature is adjuct to 50-60 C
* The ph value is regulate 4.5-5
* Add in dyeing bath 0.5-1.0 g/lt ALT EGA TC. İf need you can a add other auxiliary chemicals in bath .
* Operate the machine 5 minutes before adding dyestuff.
* Add the dyestuff which is filtered than work the machine .10-15 min İn 50-60 C bath temperature.
* Increase the bath temperature to 130 C by the 1-1,5 C/min.
* Work the machine in this 130 C temperature between 60-90 min.according to colour of light or deep.
* Reduce the bath temperature slowly to 70-80 C after finishing dyeing and than drain the water .if need make reductive washing
• Generally there is no need final cleaning operation dyeing with ALT EGA TC. For the correction of the poliester goods dyeing with poliester dyes in condition of HT( high temperature ) 0.5-1.0 g/lt ALT EGA TC at 125-135 C work wachine 1 hour.and then apply below washing process.
0.5-1.0 g/lt ALT EGA TC
1.0-2.0 g/lt sodium hydrosülfite
3.0-5.0 g/lt sodium hydroxide (35 Be)
Temperature : 70 C
Time : 10-15 min.

General usage is recomended below
For diepersant : 0.5-1.0 g/lt
For egalizator : 1.0-2.0 g/lt
Extraction of dye : 1.5-3.0 g/lt

STORAGE LIFE : Original package and normal temperature 6 month
PACKAGING : 60 Kg plastic carboys and 120 kg plactic barrelsWarning : All above information is best of our knowledge obtained during process and research.Every user of
our products should verify the data under his own conditions

Concentrate dispersion and egalize material
PRODUCTION SPECIFICATION
Chemical Composition : Combination of suitable non-ionic ether and esters
Ionic Character : Non-ionic
Appearence : Light yellow clear,voscous liquid
Ph : 6-7

PROPERTIES : * ALT EGA is a perfec disperse and egalize material
* It is foam regulated.
* It is supply uniform leveling dispers dye in poliester dyeing İndantren and reactive dye in cottons dyeing ,kationic dye goups in acrilic dyeing, acid,crom and metal complex dyes inwool dyeing baths.
* It is prevent aglomeration and waste on dying equipment
* It is proved perfect smooh dyeing handle.
* It is prevent formation of oligomer.
* Its high stability dispers and egalize metaril so,it is perfect work in high temperature and high pressure for dyeing poliester and their mixtures.
* There is needlessness washing process after dyeing because of prevent formation of oligomer.
* It is mix with water in all ratio.
* It is used with non-ionic,anionic and cationic dyes , auxiliarychemicals ,acids,salt etc.
* It is used with all kind of carrier.
* It is used for dyeing knitting ,weawing fabrics, bobbin, carpet and fibres dyeing.

APPLICATION* The bath temperature is adjuct to 50-60 C
* The ph value is regulate 4.5-5
* Add in dyeing bath 0.5-1.0 g/lt ALT EGA. İf need you can a add other auxiliary chemicals in bath .
* Operate the machine 5 minutes before adding dyestuff.
* Add the dyestuff which is filtered than work the machine .10-15 min İn 50-60 C bath temperature.
* Increase the bath temperature to 130 C by the 1-1,5 C/min.
* Work the machine in this 130 C temperature between 60-90 min. according to colour of light or deep.
* Reduce the bath temperature slowly to 70-80 C after finishing dyeing and than drain the water .if need make reductive washing

• Generally there is no need final cleaning operation dyeing
with ALT EGA . For the correction of the poliester goods dyeing with poliester dyes in condition of HT( high temperature ) 0.5-1.0 g/lt ALT EGA at 125-135 C work wachine 1 hour. and then apply below washing process.
0.5-1.0 g/lt ALT EGA
1.0-2.0 g/lt sodium hydrosülfite
3.0-5.0 g/lt sodium hydroxide (35 Be)
Temperature : 70 C
Time : 10-15 min.
General usage is recomended below
For diepersant : 0.5-1.0 g/lt
For egalizator : 1.0-2.0 g/lt
Extraction of dye : 1.5-3.0 g/lt

STORAGE LIFE : Original package and normal temperature 6 month
PACKAGING : 60 Kg plastic carboys and 120 kg plactic barrels

Concentrate dispersion and egalize material
PRODUCTION SPECIFICATION

Chemical Composition : Combination of suitable non-ionic ether and esters
Ionic Character : Non-ionic
Appearence : Light yellow clear,voscous liquid
Ph : 6-7

PROPERTIES : * ALT DIS EGA is a perfec disperse and egalize material
* It is foam regulated.
* It is supply uniform leveling dispers dye in poliester dyeing İndantren and reactive dye in cottons dyeing ,kationic dye goups in acrilic dyeing, acid,crom and metal complex dyes inwool dyeing baths.
* It is prevent aglomeration and waste on dying equipment
* It is proved perfect smooh dyeing handle.
* It is prevent formation of oligomer.
* Its high stability dispers and egalize metaril so,it is perfect work in high temperature and high pressure for dyeing poliester and their mixtures.
* There is needlessness washing process after dyeing because of prevent formation of oligomer.
* It is mix with water in all ratio.
* It is used with non-ionic,anionic and cationic dyes , auxiliary chemicals ,acids,salt etc.
* It is used with all kind of carrier.
* It is used for dyeing knitting ,weawing fabrics, bobbin, carpet and fibres dyeing.

APPLICATION * The bath temperature is adjuct to 50-60 C
* The ph value is regulate 4.5-5
* Add in dyeing bath 0.5-1.0 g/lt ALT DIS EGA. İf need you can a add other auxiliary chemicals in bath .
* Operate the machine 5 minutes before adding dyestuff.
* Add the dyestuff which is filtered than work the machine 10-15 min İn 50-60 C bath temperature.
* Increase the bath temperature to 130 C by the 1-1,5 C/min.
* Work the machine in this 130 C temperature between 60-90 min.according to colour of light or deep.
* Reduce the bath temperature slowly to 70-80 C after finishing dyeing and than drain the water .if need make reductive washing

• Generally there is no need final cleaning operation dyeing
with ALT DİS EGA . For the correction of the poliester goods dyeing with poliester dyes in condition of HT( high temperature )
0.5-1.0 g/lt ALT DİS EGA at 125-135 C work wachine 1 hour.
and then apply below washing process.0.5-1.0 g/lt ALT DIS EGA
1.0-2.0 g/lt sodium hydrosülfite
3.0-5.0 g/lt sodium hydroxide (35 Be)
Temperature : 70 C
Time : 10-15 min.
General usage is recomended below
For diepersant : 0.5-1.0 g/lt
For egalizator : 1.0-2.0 g/lt
Extraction of dye : 1.5-3.0 g/lt
STORAGE LIFE : Original package and normal temperature 6 month
PACKAGING : 60 Kg plastic carboys and 120 kg plactic barrels

Concentrate dispersion and egalize material
PRODUCTION SPECIFICATION

Chemical Composition : Combination of suitable non-ionic ether and esters
Ionic Character : Non-ionic
Appearence : Light yellow clear,voscous liquid
Ph : 6-7

PROPERTIES : * ALT DIS OZ is a perfec disperse and egalize material
* It is foam regulated.
* It is supply uniform leveling dispers dye in poliester dyeing İndantren and reactive dye in cottons dyeing ,kationic dye goups in acrilic dyeing, acid,crom and metal complex dyes inwool dyeing baths.
* It is prevent aglomeration and waste on dying equipment
* It is proved perfect smooh dyeing handle.
* It is prevent formation of oligomer.
* Its high stability dispers and egalize metaril so,it is perfect work in high temperature and high pressure for dyeing poliester and their mixtures.
* There is needlessness washing process after dyeing because of prevent formation of oligomer.
* It is mix with water in all ratio.
* It is used with non-ionic,anionic and cationic dyes , auxiliary chemicals ,acids,salt etc.
* It is used with all kind of carrier.
* It is used for dyeing knitting ,weawing fabrics, bobbin, carpet and fibres dyeing.

APPLICATION * The bath temperature is adjuct to 50-60 C
* The ph value is regulate 4.5-5
* Add in dyeing bath 0.5-1.0 g/lt ALT DIS OZ. İf need you can a add other auxiliary chemicals in bath .
* Operate the machine 5 minutes before adding dyestuff.
* Add the dyestuff which is filtered than work the machine .10-15 min İn 50-60 C bath temperature.
* Increase the bath temperature to 130 C by the 1-1,5 C/min.
* Work the machine in this 130 C temperature between 60-90 min.according to colour of light or deep.
* Reduce the bath temperature slowly to 70-80 C after finishing dyeing and than drain the water .if need make reductive washing
• Generally there is no need final cleaning operation dyeing with ALT DIS OZ. For the correction of the poliester goods dyeing with poliester dyes in condition of HT( high temperature ) 0.5-1.0 g/lt ALT DIS OZ at 125-135 C work wachine 1 hour.and then apply below washing process.0.5-1.0 g/lt ALT DIS OZ 1.0-2.0 g/lt sodium hydrosülfite 3.0-5.0 g/lt sodium hydroxide (35 Be)
Temperature : 70 C
Time : 10-15 min.

General usage is recomended below
For diepersant : 0.5-1.0 g/lt
For egalizator : 1.0-2.0 g/lt
Extraction of dye : 1.5-3.0 g/lt

STORAGE LIFE : Original package and normal temperature 6 month
PACKAGING : 60 Kg plastic carboys and 120 kg plactic barrelsWarning : All above information is best of our knowledge obtained during process and research.Every user of
our products should verify the data under his own conditions.

Concentrate dispersion and egalize material
PRODUCTION SPECIFICATION

Chemical Composition : Combination of suitable non-ionic ether and esters
Ionic Character : Non-ionic
Appearence : Light yellow clear,voscous liquid
Ph : 6-7

PROPERTIES :* ALT DIS YT is a perfec disperse and egalize material
* It is foam regulated.
* It is supply uniform leveling dispers dye in poliester dyeing İndantren and reactive dye in cottons dyeing ,kationic dye goups in acrilic dyeing, acid,crom and metal complex dyes inwool dyeing baths.
* It is prevent aglomeration and waste on dying equipment
* It is proved perfect smooh dyeing handle.
* It is prevent formation of oligomer.
* Its high stability dispers and egalize metaril so,it is perfect work in high temperature and high pressure for dyeing poliester and their mixtures.
* There is needlessness washing process after dyeing because of prevent formation of oligomer.
* It is mix with water in all ratio.
* It is used with non-ionic,anionic and cationic dyes , auxiliary chemicals ,acids,salt etc.
* It is used with all kind of carrier.
* It is used for dyeing knitting ,weawing fabrics, bobbin, carpet and fibres dyeing.

APPLICATION * The bath temperature is adjuct to 50-60 C
* The ph value is regulate 4.5-5
* Add in dyeing bath 0.6-1.2 g/lt ALT DIS YT. İf need you can a add other auxiliary chemicals in bath .
* Operate the machine 5 minutes before adding dyestuff.
* Add the dyestuff which is filtered than work the machine .10-15 min İn 50-60 C bath temperature.
* Increase the bath temperature to 130 C by the 1-1,5 C/min.
* Work the machine in this 130 C temperature between 60-90 min. according to colour of light or deep.
* Reduce the bath temperature slowly to 70-80 C after finishing dyeing and than drain the water .if need make reductive washing
• Generally there is no need final cleaning operation dyeing with ALT DIS YT.For the correction of the poliester goods dyeing with poliester dyes in condition of HT( high temperature )
1.0-1.5 g/lt ALT DIS YT at 125-135 C work wachine 1 hour.and then apply below washing process. 1.0-1.5 g/lt ALT DIS YT  1.0-2.0 g/lt sodium hydrosülfite 3.0-5.0 g/lt sodium hydroxide (35 Be)
Temperature : 70 C
Time : 10-15 min.

General usage is recomended below
For diepersant : 1.0-1.5 g/lt
For egalizator : 1.5-2.5 g/lt
Extraction of dye : 2.0-3.0 g/lt

STORAGE LIFE : Original package and normal temperature 6 month
PACKAGING : 60 Kg plastic carboys and 120 kg plactic barrelsWarning : All above information is best of our knowledge obtained during process and research.Every user of
our products should verify the data under his own conditions.

Concentrate dispersion and egalize material
PRODUCTION SPECIFICATION

Chemical Composition : Combination of suitable non-ionic ether and esters
Ionic Character : Non-ionic
Appearence : Light yellow clear,voscous liquid
Ph : 6-7

PROPERTIES : * ALT DIS P CONZ is a perfec disperse and egalize material
* It is foam regulated.
* It is supply uniform leveling dispers dye in poliester dyeing İndantren and reactive dye in cottons dyeing ,kationic dye goups in acrilic dyeing, acid,crom and metal complex dyes inwool dyeing baths.
* It is prevent aglomeration and waste on dying equipment
* It is proved perfect smooh dyeing handle.
* It is prevent formation of oligomer.
* Its high stability dispers and egalize metaril so,it is perfect work in high temperature and high pressure for dyeing poliester and their mixtures.
* There is needlessness washing process after dyeing because of prevent formation of oligomer.
* It is mix with water in all ratio.
* It is used with non-ionic,anionic and cationic dyes , auxiliary chemicals ,acids,salt etc.
* It is used with all kind of carrier.
* It is used for dyeing knitting ,weawing fabrics, bobbin,carpet and fibres dyeing.

APPLICATION* The bath temperature is adjuct to 50-60 C
* The ph value is regulate 4.5-5
* Add in dyeing bath 0.6-1.2 g/lt ALTDIS P CONZ İf need you can a add other auxiliary chemicals in bath .
* Operate the machine 5 minutes before adding dyestuff.
* Add the dyestuff which is filtered than work the machine .10-15 min İn 50-60 C bath temperature.
* Increase the bath temperature to 130 C by the 1-1,5 C/min.
* Work the machine in this 130 C temperature between 60-90 min.according to colour of light or deep.
* Reduce the bath temperature slowly to 70-80 C after finishing dyeing and than drain the water .if need make reductive washing

• Generally there is no need final cleaning operation dyeing
with ALT DIS P CONZ.For the correction of the poliester goods dyeing with poliester dyes in condition of HT( high temperature ) 1.0-1.5 g/lt ALT DIS P CONZ at 125-135 C work wachine 1 hour.and then apply below washing process.1.0-1.5 g/lt ALT DIS P CONZ 1.0-2.0 g/lt sodium hydrosülfite 3.0-5.0 g/lt sodium hydroxide (35 Be)
Temperature : 70 C
Time : 10-15 min.

General usage is recomended below
For diepersant : 1.0-1.5 g/lt
For egalizator : 1.5-2.5 g/lt
Extraction of dye : 2.0-3.0 g/lt

STORAGE LIFE : Original package and normal temperature 6 month
PACKAGING : 60 Kg plastic carboys and 120 kg plactic barrelsWarning : All above information is best of our knowledge obtained during process and research.Every user of
our products should verify the data under his own conditions.

Concentrate dispersion and egalize material

PRODUCTION SPECIFICATION


Chemical Composition : Combination of suitable non-ionic ether and esters
Ionic Character : Non-ionic
Appearence : Light yellow clear,voscous liquid
PROPERTIES :* ALT DIS P is a perfec disperse and egalize material
* It is foam regulated.
* It is supply uniform leveling dispers dye in poliester dyeing İndantren and reactive dye in cottons dyeing ,kationic dye goups in acrilic dyeing, acid,crom and metal complex dyes inwool dyeing baths.
* It is prevent aglomeration and waste on dying equipment
* It is proved perfect smooh dyeing handle.
* It is prevent formation of oligomer.
* Its high stability dispers and egalize metaril so,it is perfect work in high temperature and high pressure for dyeing poliester and their mixtures.
* There is needlessness washing process after dyeing because of prevent formation of oligomer.
* It is mix with water in all ratio.
* It is used with non-ionic,anionic and cationic dyes , auxiliary chemicals ,acids,salt etc.
* It is used with all kind of carrier.
* It is used for dyeing knitting ,weawing fabrics, bobbin, carpet and fibres dyeing.

APPLICATION * The bath temperature is adjuct to 50-60 C
* The ph value is regulate 4.5-5
* Add in dyeing bath 1.0-3.0 g/lt ALT DIS P İf need you can a add other auxiliary chemicals in bath .
* Operate the machine 5 minutes before adding dyestuff.
* Add the dyestuff which is filtered than work the machine .10-15 min İn 50-60 C bath temperature.
* Increase the bath temperature to 130 C by the 1-1,5 C/min.
* Work the machine in this 130 C temperature between 60-90 min.according to colour of light or deep.
* Reduce the bath temperature slowly to 70-80 C after finishing dyeing and than drain the water .if need make reductive washing

• Generally there is no need final cleaning operation dyeing with ALT DIS P.For the correction of the poliester goods dyeing with poliester dyes in condition of HT( high temperature )
1.5-2.5 g/lt ALT DIS P at 125-135 C work wachine 1 hour.and then apply below washing process.1.5-2.5 g/lt ALT DIS P 2.0-3.5 g/lt sodium hydrosülfite 3.0-5.0 g/lt sodium hydroxide (35 Be)
Temperature : 70 C
Time : 10-15 min.

General usage is recomended below
For diepersant :1.0-1.5 g/lt
For egalizator :1.5-2.5 g/lt
Extraction of dye :2.0-3.0 g/lt

STORAGE LIFE : Original package and normal temperature 6 month
PACKAGING : 60 Kg plastic carboys and 120 kg plactic barrelsWarning : All above information is best of our knowledge obtained during process and research.Every user of
our products should verify the data under his own conditions.

Leveling agent of nylon


Dispersion and leveling material for PA and its mixtures
PRODUCTION SPECIFICATION

Chemical Composition :
Ionic Character : Anionic
Appearence : Brown ,fluid liquid
Ph : 6-7

PROPERTIES : * ALT EGA NL leveling occur of line making minimises affinity on fibres when dyeing
• ALT EGA NL reserved nylon fibres on dyeing of nylon/wool wool mixtures so its delay qickly dyeing nylon from wool
* ALT EGA NL is resistant to hard water,acids,alkalies ,electrolytic solution, reductant and oxidizing agents.
• ALT EGA NL is not occur foam also high circulation machine.
• ALT EGA NL is owner perfect leveling and migration properties.o

APPLICATION :For dyeing of PA with dyestuff  0.5-1.0 %

STORAGE LIFE : Original package and normal temperature 6 month
PACKAGING : 0 Kg plastic carboys and 120 kg plactic barrelsWarning : All above information is best of our knowledge obtained during process and research.Every user of
our products should verify the data under his own conditions.

Polimerik Kırık Önleyici
PRODUCTION SPECIFICATION
Chemical Composition : Polyacrilad based non-ionic micro emulsion
Ionic Character : Non-ionic
Appearence : Slight yellow clear fluid liquid.
Ph : 6-7
Solubility : soluble

PROPERTIES :* ALT POL TT is used crease preventative in the dying and bleaching processes all natural ans synthetic fibres
* It is contains special chemicals so, it gives brillant and fresh handle.
* It is reduce frictions of fiber-fiber and fiber metal because of its antistatic and slipper properties.
* It is provides ease sewing.
* It is suitable all ph value range and all temperature and it is used with all non-ionic materials .
* It is mix with all hot and cold water.
* It is uesd with every bleaching chemicals and optical whiter.

APPLICATIONS :According to type of fabric and fibres, it is used 1.5-3.0 % ALT POL TT shoul be add in dyeing bath firstly before other auxiliary chemicals and stirr 5-10 minutes in machine.

STORAGE LIFE : Original package and normal temperature 6 month
PACKAGİNG : 60 Kg plastic carboys and 120 kg plactic barrels
Warning : All above information is best of our knowledge obtained during process and research.Every user of
our products should verify the data under his own conditions.

PRODUCTION SPECIFICATION

Chemical Composition : Combination of fat and fatty acid derivatives
Ionic Character : Anionic
Appearence : yellow viscose liquid.Ph :6-7
PROPERTIES : ALT OIL TX is used crease preventative in the dying and Pre-treatmant processes all natural ans synthetic fibres
* It is resistant to high ph value, high saltiness ,and high temperature.It gives to fibre a soft ,slippery handle and so it prevents the crease to be seen.
* It is dissolve in water and there is no aglomeration in dyeing of reactive turquoise.
* It can be used in jet machines.It provides a homogeneous distribution of molecules in dyeing bath and helps the absorption to perfect.

APPLICATIONS : cotton and viscone :0.5-1.0 g/lt Wool and polyamide :0.5-1.0 g/lt Poliester :0.3-0.5 g/lt

STORAGE LIFE : Original package and normal temperature 6 month It must protect from hot and cold.
PACKAGİNG : 60 Kg plastic carboys and 120 kg plactic barrelsWarning : All above information is best of our knowledge obtained during process and research.Every user of
our products should verify the data under his own conditions.